Question: We manufacture two-part epoxy adhesives that are normally used by customers at ambient temperatures. We don’t completely understand why we always seem to get higher strengths if we cure them at higher temperatures. Is it a different type of curing?



Answer: It is difficult to give you an exact answer without the full details of the adhesive or what type of hardener you use for the epoxy. However, I can make some comments and generalizations about this type of adhesive.

Compared to some other types of structural adhesives, such as cyanoacrylates or reactive acrylics, epoxies are highly crosslinked structures and tend to become highly viscous very early in their cure cycle. The result is that the molecules’ mobility becomes restricted, which limits their ability to collide and react.

Is not unusual to see a lot of unreacted epoxy when curing is carried out at moderate temperatures. Heat has two effects: it lowers the viscosity and increases the reaction rate. A good way to observe this is to perform differential scanning calorimetry (DSC) on your cured adhesive. DSC measures the energy absorbed or released as the adhesive is ramped up from low to high temperatures.

In the case of the adhesive cured at ambient temperature, you will normally see an exothermic peak (heat released) during the scan as the remaining epoxy cures; the area under this peak gives you an estimate of the amount of unreacted epoxy in the sample. When an adhesive is fully cured at higher temperatures, this peak will not be observed. Heat-cured adhesives give the maximum adhesive strength and physical properties, plus enhanced heat and fluid resistance. It is common to have long heat cure cycles for very high strength epoxy adhesives.

Did you enjoy this article? Click here to subscribe to Adhesives & Sealants Industry Magazine.

Dunn

Q&A Exchange is written by Dave Dunn, Ph.D., of F.L.D.Enterprises, a technical consultancy and full-service industrial market-research firm specializing in the adhesives, sealants, specialty rubbers and plastics fields. Dave is a former vice president and director of Loctite Corp. and has spent many years in troubleshooting adhesive and sealant problems. Questions for publication should be directed to him at 242 Trails End, Aurora OH 44202; phone 330-562-2930; fax (330) 247-1690; or email DrDave242@windstream.net .

Recent Articles by Dave Dunn

You must login or register in order to post a comment.

Multimedia

Videos

Podcasts

Environmentally Friendly Manufacturing

Edward Gotch, president of Emerald Kalama Chemical, talks about embracing sustainability with Susan Sutton, editor-in-chief.

More Podcasts

THE MAGAZINE

Adhesives & Sealants Industry Magazine

ASI May 2013 cover 100x133

2013 May

The 2013 May Adhesives and Sealants Industry Magazine includes articles about PPG and Bostik, as well as a Q&A about polyurethane. Check it out today!

Table Of Contents Subscribe

THE ADHESIVES STORE

handbook-sealant-tech.gif
Handbook of Sealant Technology

The Handbook of Sealant Technology provides an in-depth examination of sealants, reviewing their historical developments and fundamentals, adhesion theories and properties, and today’s wide range of applications.

More Products

asi1211p_Cover-DE.gifASI's Buyers' Guide

Annual purchasing resource for equipment used in the manufacture/formulation of adhesives, sealants, pressure sensitives, tapes and labels and for application of finished adhesives. 

Clear Seas Research

With access to over one million professionals and more than 60 industry-specific publications, Clear Seas Research offers relevant insights from those who know your industry best. Let us customize a market research solution that exceeds your marketing goals.

STAY CONNECTED

facebook_40px twitter_40  youtube_40pxlinkedin_40