Adhesives Mag logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Create Account
  • Sign Out
  • My Account
Adhesives Mag logo
  • NEW PRODUCTS
  • NEWS
    • Adhesives & Sealants Headlines
    • Mergers/Acquisitions
    • Market Trends
    • TOP 20
  • TOPICS
    • Finished Adhesives and Sealants
    • Pressure-Sensitive Adhesives (PSAs)
    • Coatings
    • Raw Materials and Chemicals
    • Materials Handling/Processing
    • Meter/Mix/Dispense
    • Curing
    • Testing/Quality Control
    • Packaging of Adhesives & Sealants
    • Converting/Packaging
    • Composites
    • Sustainability
  • EVENTS
    • ASI Academy
    • Events Calendar
  • COLUMNS
    • European Perspectives
    • Strategic Solutions
    • Supply Chain Strategies
    • Tape Talk
  • MULTIMEDIA
    • Videos
    • Podcasts
    • Webinars
    • eBooks
  • EXPLORE
    • Adhesives in Action
    • Blog
    • ASI Store
    • Industry Links
    • Market Research
    • Classifieds
  • DIRECTORIES
    • Buyers' Guide
    • Global Adhesives & Sealants Directory
    • Raw Materials, Chemicals, Polymers and Additives Handbook
    • Equipment Handbook
    • Distributor Directory
  • EMAGAZINE
    • EMAGAZINE
    • ARCHIVE ISSUES
    • ADVERTISE
      • Custom Content & Marketing Services
    • CONTACT
  • SIGN UP!

Redispersible Powders for Sealing Slurries

June 1, 2004
Mixing two-component flexible cementitious sealing slurries on-site immediately before use may soon become a thing of the past. A redispersible polymer powder has been developed that enables the formulation of one-component products. Polymer powders of this type can also be used successfully, in other ‘elastic' applications, such as highly flexible tile adhesives

The effects of polymer dispersions on the physical and chemical properties of flexible cementitious sealing slurries are well known.1 The resulting products have been used for many years as surface-protection systems.2 Second-generation sealing slurries of this type are characterized by their high polymer fraction with the polymer-cement (p/c) ratio being typically 0.8 or more. The polymer, which ensures that the membrane remains flexible down to low temperatures, must have a very low glass-transition temperature (Tg) (typically in the region -5 to -60°C). The technical properties of this type of building material are described elsewhere.1-2

Figure 1. The action of spray additives in the spray drying of aqueous polymer dispersions

Powdered Polymeric Starting Material

Until recently, all commercially available low-temperature flexible sealing slurries were two-component systems. This meant that, immediately prior to use, the user had to mix a powdered component with a liquid component on-site. Both logistic considerations (reduction in freight volume, no need to protect against freezing during storage, simplified disposal of containers) and the improved handling properties (ready-made powdered product that can be mixed to the required consistency by simply adding water, thus making preparation more reproducible and less prone to error), led to considerable effort in developing a suitable single-component cementitious slurry product. The main difficulty in this development work was the availability of a powdered polymer that exhibited adequate low-temperature flexibility and good processing properties, especially with regard to the drying of the slurry coat after application.

The aim of this article is twofold: to explain the difficulties in producing a redispersible powder with adequate low-temperature flexibility, and to present a new solution to this problem, including a description of the associated physical and chemical characteristics. The use of powdered products of this kind in other "elastic" applications, such as flexible tile adhesives, will also be discussed.

Figure 2. Fluorescence microscopy image of an acrylate dispersion powder recorded with a confocal laser-scanning microscope

Redispersible Powders from Drying Aqueous Polymer Dispersions

Redispersible powders3-7 are usually made by carefully drying aqueous polymeric suspensions in a spray drier.8 Typically, drying temperatures are 120-200°C at the drier entrance and 60-80°C at the drier exit (the cooling being due to evaporation of the water of dispersion). At such high drying temperatures there is a risk that a soft polymer (e.g., one with a Tg well below 0°C) will undergo irreversible particle-particle coalescence and film formation during the drying process. Initial deterioration of this type often results in formation of undesirable large size agglomerates and poor redispersion properties when water is added on the job site. However, since it is only the redispersible fraction of a dispersion powder that modifies the properties of the building material (a fact especially evident whenever the dispersion powder alone is responsible for binding9), poor redispersibility can only be compensated for by the undesirable step of increasing the amount of powder used.

Spray Additives Improve Redispersion of the Dry Powder

Generally, premature film formation of the polymer particles can be prevented by including hard, water-soluble additives (spray additives) to the dispersed binding agent prior to the drying step (see Figure 1).

The spray additive distributes itself between the continuous aqueous phase and the surface of the dispersed particles. Since the spray dries within seconds, the distribution of particles at that time becomes frozen in, with the spray additive acting as an inter-particle spacer. Irreversible coalescence of the polymer particles is thus prevented. If the dried powder is subsequently mixed with water again, even low-level shear is sufficient to cause the spray additive to dissolve completely, releasing the essentially unchanged primary dispersion particles. The polymer powder is thus re-dispersible again.

The validity of this model has been established with microscopic measurements. Fluorescence microscopy using a confocal laser-scanning microscope (CLSM) is a non-destructive optical technique that can generate high-resolution images of very thin, well-defined sections of a prepared specimen. The method is, therefore, especially suited to imaging the interior of particles in the dispersion powder.

Figure 2 shows a CLSM image of a BASF product after embedding in silicone oil. In addition, a powder sample was ground in a mortar at -120°C and the fragments examined in a scanning electron microscope.

Figure 3. Tensile strain test on redispersion films — dependence of extension on glass transition temperature and spray additive

Preparation of Dispersion Polymer/Spray Additive Mixtures

Four model polymer dispersions were prepared using a standard semi-batch polymerization process. The dispersions differed in their styrene-acrylate ratio and therefore had correspondingly different Tgs. All other experimental parameters were kept constant to assist the comparison of results.

The spray additives used included an aryl sulfonate-based low-molecular-weight condensation product and a polyvinyl alcohol (PVA) with a degree of saponification of approx. 88% and a weight-average molecular mass of approx. 26,000 g/mol.

Spray additive solutions were stirred into the dispersions and mixtures were then adjusted to a solids content of 30% using added deionized water. Spray drying was performed in a laboratory apparatus with maximum 2 kg material/hr throughput capacity, using a binary nozzle atomizer under standard conditions.

A qualitative assessment was made of the redispersibility of the polymer powders based on the amount of sediment that formed during a 72-hour redispersion period with a solid fraction of 30% w/w.

Figure 4. Tensile stress testing of redispersion films — dependence of maximum tensile strength on glass transition temperature and spray additive

Tensile Strain Test Results

To compare the flexibility of the polymer powders, air-dried films were tested using a tensile strain experiment. All powders were redispersed in water in the ratio 30% w/w and left to form a film at room temperature. The free polymer films achieved their final hardness within two weeks at the most. Film samples were pulled in a commercial tensometer at temperatures of 25 to -5°C, until fracture.

At a temperature of 25°C, the elongation at break of these redispersion films -and thus their elasticity - was essentially independent of the Tg. Effects first become observable at lower temperatures. At -5°C, redispersible powders with a Tg above approx. 10°C are essentially inflexible. Soft powders with a Tg under about 5°C are still elastic at this temperature, the extent of elasticity being determined by the spray additive (see Figure 3).

The fact that the redispersion powder with a Tg of -33°C at a test temperature of -5°C is not more flexible than that with a Tg of -16°C is presumably a result of a small amount of prior film formation during the spray drying process.

In contrast, the maximum tensile strength (stress) is solely determined by the difference between the glass transition temperature of the polymer and the measurement temperature, and it falls monotonically as a function of decreasing Tg (see Figure 4). The type of spray additive used has no significant effect on the tear strength.

Figure 5. Temperature dependence of the tensile moduli of polymer films — the influence of the spray additive and spray drying (Tg = –35°C, from DSC –33°C)

Spray Additive Influences the Temperature Dependence of the Tensile Modulus

The qualitative property of a polymer film known as ‘flexibility' is associated with the material's tensile strength and its elongation at break. However, this behavior is best interpreted in terms of the temperature dependence of the film's tensile modulus. The tensile modulus can be interpreted as the initial gradient of the stress-strain (load-extension) curve from a simple tensile loading test, and comprises an elastic part (storage modulus E') and a viscous part (loss modulus E").

To measure these quantities, the initial dispersions and the polymer/spray additive mixtures were left to form a film at room temperature both before and after spray drying. The temperature dependence of the polymer film's storage and loss moduli were then determined in a dynamic mechanical analyzer.11

The influence of the aryl-sulfonate-based spray additive is demonstrated in Figures 5-6.



Figure 6. Temperature dependence of the tensile moduli of polymer films — the influence of the spray additive and spray drying (Tg = +13°C, from DSC +14°C)
The low-molecular-weight (hard) aromatic spray additive is fully miscible with the styrene-acrylate copolymer; as a result, the tensile moduli of the polymer film at temperatures above the polymer Tg is increased by several orders of magnitude. Eventually, an essentially temperature-independent region (plateau) is achieved due to the physical crosslinking of the dispersion polymer particles by the spray additive. This phase structure is also retained after spray drying; the temperature dependence of E' and E" are practically identical before and after spray drying. The redispersion film, therefore, demonstrates the desired rubber-like elasticity that is responsible for the flexibility and strength observed in the elongation at break experiment.

Very different behavior is observed when the partially saponified polyvinyl alcohol spray additive is used. The much greater molecular mass of the polyvinyl alcohol means that this additive is effectively immiscible with most copolymers, including the styrene-acrylate copolymers used in the present study. The two polymer phases, therefore, remain separated in the mixture; as a result, a second glass transition - that of the polyvinyl alcohol - is observed at around 60-70°C. In this temperature range, the tensile moduli decrease with increasing temperature (see Figure 6).

The absence of physical crosslinking means that there is only minimal cohesion within the redispersion film when subjected to thermal or tensile stress. The low level restoring forces are also manifest in the low flexibility observed in the tensile strain test (see Figure 3).

These experimental observations are of direct relevance to product applications characterized by a high polymer fraction and a desired high degree of low-temperature flexibility. Examples of such applications are flexible sealing slurries and flexible tile adhesives, both of which are discussed in greater detail in the following two sections.

Tensile Testing of Single-Component Sealing Slurries

Each of the six redispersible powders described was used to manufacture a single-component (‘one-pack') sealing slurry using the simplest possible formulation (see Table 3).

Figure 7. Tensile testing of low-temperature flexible single-component (‘one-pack’) sealing slurries — dependence of the tear strength on the glass-transition temperature and the spray additive
The polymer-cement ratio (p/c) was 0.8, with total polymer content of approximately 17% in all dry mixtures. Mixing water level was adjusted to produce a slurry with a consistency suitable for application with a roller.

Once mixed for use, each sealing slurry was spread wet-on-wet in two to three coats onto an inert polyethylene sheet (application rate: 3 kg/m2), left to dry for 24 hours and then peeled off as a film. The films were then stored for a further 14 days in a standard reference atmosphere. The tensile breaking strength and the elongation at break of each slurry film was then measured at room temperature, 10°C and -5°C (see Figures 7-8).

Figure 8. Tensile testing of low-temperature flexible single-component (‘one-pack’) sealing slurries — dependence of the elongation at break on the glass-transition temperature and the spray additive
The room temperature tests demonstrate the decreasing tensile tear strength and the increasing elongation at break of the sealing slurries as the Tg decreases. The reason why the polyvinyl alcohol/acrylate powders exhibit lower tensile strength and reduced elongation at break compared to the aryl sulfonate containing samples is that the former has a lower cohesion due to the incompatibility of the polyvinyl alcohol and the acrylate copolymer.

As the investigations of the elongation at break at 10°C and, in particular, at -5°C show, a sealing slurry will only exhibit sufficient flexibility if the Tg of the polymeric component is far enough below the measurement temperature. However, the price paid for this effect is the significant reduction in the inherent strength of such a product (see the results for the softest polymer in Figure 7). Even at the lower measurement temperatures, the polyvinyl alcohol-containing acrylate powders are again characterized by their lower tensile strengths and lower extensibility compared to the aryl sulfonate samples.

From the results discussed in this section, the sealing slurry with the most balanced set of properties in terms of inherent strength and low-temperature flexibility is the aryl sulfonate redispersible powder with a glass transition temperature of -16°C.



Bond Strengths of Flexible One-Component Tile Adhesives

Two aryl-sulfonate-modified acrylate powders with Tgs of +14°C and -16°C (A1 and C1, respectively) were used in the preparation of powdered flexible tile adhesives. Testing of the corresponding polyvinyl-alcohol-modified powders was not possible because the bond strengths of the corresponding tile adhesive formulations were far too low.

As with the sealing slurries, the simplest possible recipe was used for the investigations of the polymer-modified cementitious tile adhesives (see Table 4).

To understand the effect of polymer content in the formulation, the polymer-cement ratio of the dry mixture was varied between 0.04 and 0.31, corresponding to a polymer fraction of between approx. 1.5 and 12% w/w in the tile adhesive. For comparison purposes, a common, commercially available EVA-based polymer powder recommended for this purpose was also tested (Tg = -5°C; contains polyvinyl alcohol; EVA = ethylene vinylacetate).

The amount of mixing water required was that which gave the best workability coupled with sufficient stability of the tile on the test substrate. As shown in Figure 9, the amount of water required was found to decrease with increasing p/c with the acrylate powder systems but was approximately constant with the EVA-based powder. As expected, the differences between the two product groups are marginal at very low polymer fractions.

Tile adhesive bond strengths were determined using the old DIN 18 156 standard (tile pulloff test) on samples with p/c ratios of 0.04 and 0.23 (corresponding to a polymer fraction of 1.5% w/w and 10% w/w, respectively). Bond strengths were measured under four conditions: after 28 days dry storage at room temperature ("standard reference atmosphere"); after 28 days in the standard reference atmosphere followed by additional high-temperature storage at 70°C; after 7 days in the standard reference atmosphere and then 21 days wet storage; and after 7 days in the standard reference atmosphere followed by freeze-thaw cycling.

The failure pattern observed during these tests was always either cohesive failure or concrete substrate breakout and never adhesive failure. The measured bond strengths, therefore, represent minimum values and reflect the inherent strength of the tile adhesive. Their magnitude may, however, also be a result of the reduced amount of water required by these modified materials.

Figure 9. The amount of water required for ‘one-pack’ flexible tile adhesives

Bond Strength and Freeze-Thaw Cycling

The bond strength results shown in Figure 10 demonstrate that the differences between the three test powders are slight at low polymer fractions. At the higher polymer level tested (p/c = 0.23), in spite of the lower Tg and high inherent flexibility, C1 yielded bond strengths that were indeed somewhat less than the higher Tg polymer A1 but, importantly, were comparable to the harder commercial EVA-based powder - with its much weaker ability to impart flexibility.

As the experiments on the sealing slurries showed (see Figure 8), the addition of a sufficient quantity of soft acrylate powder C1 results in a dramatic increase in the flexibility of the cementitious compound material. The lower inherent strength of the polymer is the reason for the reduced bond strength compared with the harder polymer A1 (see Figure 10). This effect is compensated to some extent by the reduced amount of water required by the acrylate-containing formulations (see Figure 9). It is noteworthy that, compared with the EVA-based product, the two acrylate-containing powders offer significant advantages when subjected to the particularly critical freeze-thaw cycling test.

The choice of the right acrylate powder for flexible and highly flexible tile adhesives depends upon the desired material properties. If a high inherent strength is of primary importance for an application, then the harder powder A1 is certainly preferable. If the user attaches greater weight to a product with good (low-temperature) flexibility and adequate inherent strength (e.g., when tiling on a substrate that may be subject to movement), a softer powder such as C1 is the material of choice.

Figure 10. Bond strengths of flexible ‘one-pack’ tile adhesives on concrete*

* Normal storage: 28d standard reference atmosphere; Wet storage: 7d standard reference atmosphere + 21d wet storage; High-temp. storage: 28d standard reference atmosphere + 14d 70°C + 1d standard reference atmosphere; Freeze-thaw cycling: 7d standard reference atmosphere + 21d wet storage + 25 “–15°C/Water” cycles)

Summary

The present work provides insights to the challenges associated with manufacturing soft redispersible polymer powders (i.e., ones that are flexible at low temperatures). By using a new spray drying additive technology, the elastic properties of a soft acrylate dispersion can be retained in the resulting redispersible acrylate powder. Powder products of this type can be used successfully in ‘elastic' applications such as flexible cementitious sealing slurries and (highly) flexible tile adhesives. In the latter, high bond strengths are combined with excellent resistance to freeze-thaw stress and exceptionally good flexibility, even at low temperatures.

For more information on redispersible polymer powders, contact Luke Egan, eganl@basf.com .

References

1 Angel, M.; Denu, H.-J. Dichtungsschlämmen für den Betonoberflächenschutz [Sealing slurries for protecting concrete surfaces]. Farbe&Lack 103 (1997), No. 8, p. 92.

2 Volkwein, A..; Petri, R.; Springenschmid, R. Oberflächenschutz von Beton mit flexiblen Dichtungsschlämmen - Teil 1 [Concrete surface protection using flexible sealing slurries - Part 1]. Betonwerk und Fertigteiltechnik 54 (1988), No. 8, p. 30. b) Volkwein, A..; Petri, R.; Springenschmid, R. Oberflächenschutz von Beton mit flexiblen Dichtungsschlämmen - Teil 2 [Concrete surface protection using flexible sealing slurries - Part 2]. Betonwerk und Fertigteiltechnik 54 (1988), No. 9, p. 72.

3 Schulze, J. Redispersionspulver im Zement [Redispersible powders in cement]. TIZ-Fachberichte 109 (1985) No. 9, p. 698.

4 Rietz, U.; Dispersionspulver, Herstellung und Verwendung [Redispersible powders: manufacture and use]. Chem. Tech. makromol. Stoffe (FH-Texte, 12. Koll. FH Aachen) 53 (1987), p. 85.

5 Walters, D.G. VAE Redispersible-Powder Hydraulic-Cement Admixtures. Concrete Int. 14 (1992) No. 4, p. 30.

6 Tsai, M.C.; Burch, M.J.; Lavelle, J.A. Acrylic Dry Polymer Modified High Solids Cementicious Coatings. Proc. Water-Borne Higher-Solids Powder Coat. Symp. (1993), p. 322.

7 Denu, H.-J.; Pakusch, J. Ein neues Dispersionspulver mit integrierter Bindemittel- und Verlaufsfunktion [A new redispersible powder with integrated binding and leveling properties]. European Coatings Show (Nürnberg 1999) Bauchemiekongreß.

8 Armbruster, W. Die Zerstäubungstrocknung [Spray drying]. Chem. App. Verfahrenstechnik 93 (1969) No. 12, p. 469.

9 Dörr, H.; Lohmann, W. Ohne Wasser geht's auch - optimales Formulieren und Produzieren von Dispersions-Pulverfarben. [Doing without water - optimized formulations and the production of dispersible powder pigments]. Farbe&Lack 101 (1995), No. 8, p. 708.

10 Richardson, M.J. Comprehensive Polymer Science Vol. I. Hrsg. C. Booth, C. Price, Pergamon Press Oxford (1989), p. 867.

11 Zosel. A. Lack- und Polymerfilme - viskoelastische Qualitätsmerkmale [Paint and polymer films - viscoelastic quality characteristics). Hrsg. U. Zorll, C.R. Vincentz Verlag Hannover (1996), p. 21.

12 Mächtle, W. Coupling Particle Size Distribution Technique. Angew. Makromol. Chem. 162 (1988), p. 35.

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • linked network nodes

    Using the Power of AI for Adhesive and Sealant Formulation

    With the help of software solutions, adhesive formulators...
    Finished Adhesives and Sealants
    By: Karen Parker
  • ASI top 20 global manufacturers

    2025 ASI Top 20: Leading Global Adhesives and Sealants Manufacturers

    ASI's annual ranking of the top 20 global adhesive and...
    Adhesives and Sealants Topics
    By: Karen Parker
  • science test tubes

    2026 Adhesives and Sealants Raw Materials Roundup

    After more than two years of contraction, the...
    Raw Materials and Chemicals
    By: Karen Parker
Manage My Account
  • eMagazine Issues
  • Newsletters
  • Online Registration
  • Manage My Preferences
  • Subscription Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the Adhesives and Sealants Industry audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of Adhesives and Sealants Industry or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • Assembly automation for medical device manufacturing
    Sponsored byNordson EFD

    Three Proven Principles Powering Quality Assembly

Popular Stories

Image of a blue bar chart with arrow pointing up

Iran War and Logistics Challenges Impact Adhesives and Sealants Pricing

news on internet screen

H.B. Fuller and Ancora Holdings Clash Over Proposed Medical Adhesives Acquisition

Aerial picture of a chemical facility

DELO Reports Record Revenue for Fiscal Year

ASI Top 20 website

Events

June 15, 2026

Adhesive and Sealant Council Executive Leadership Conference

This annual event provides current and future leaders in the adhesives and sealants industry with the opportunity to expand their knowledge and network with peers.

September 14, 2026

Women in Chemicals Conference

Organized by Women in Chemicals, this landmark conference will offer opportunities for networking, learning, and professional development. With a diverse array of sessions, workshops, and social events, participants can expect a dynamic program designed to empower and inspire.

View All Submit An Event

Products

Structural Adhesives: Properties, Characterization and Applications

Structural Adhesives: Properties, Characterization and Applications

See More Products

ASI CASE EBOOK

ASI raw materials roundup

Related Articles

  • ROHM AND HAAS: Redispersible Powders

    See More
  • Mixing Flights

    Rotary Batch Mixer Blends Wood Powders for Plywood Adhesives

    See More
  • Ask Dr. Dave: We're concerned about using 100% solids methacrylate-based sealants for sealing metal joints.

    See More

Related Directories

  • Seal Bond

    Custom formulation and manufacturing of adhesives, sealants, and coatings. Toll manufacturing, private label, custom coloring, and application and process development.
×

Keep the info flowing with our newsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Manufacturing Division
    • Store
    • Want More
  • SIGN UP TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing