Polymers Microsite
  Home
  ASI Green
  Subscribe
  eNewsletter Subscription
  Subscription Customer Service
  Updates
  Calendar of Events
  Call for Papers
  Features
  Columns
  Today's Headlines
  Price Adjustments
  New Products
  Ad Index
  Podcasts
  Ask Dr. Dave
  ASI Blog
  Online Exclusives
  Adhesives in the News
  Resources
  Books
  Archives
  Digital Edition Archives
  Classified Ads
  Career Center
  Tech ManufactureXPO
  Industry Links
  Online Solutions Web Seminars
  This to That
  Services Marketplace
  E-Newsletter Archives
  Green Opportunities E-News Archives
  Market Research
  Literature Showcases
  Glossaries
  Directories
  ASI Info
  Media Kit
  Contact Us
  Sales Staff
  Reprints
  List Rental
Search in: EditorialProductsCompanies

About Polymers
A polymer consists of a long molecular chain made of equal units (monomers). The Freedonia Group projects that U.S. natural polymer demand is expected to grow 5.9% annually to $3.6 billion in 2010. Find out the latest information on polymers and their use in adhesive and sealant formulations by clicking on the links below.


Advanced Polymer Design for Adhesives
by Dr. Cornelis Beyers
Dr. Stefan Kirsch
Dr. Petra Schöcker
Dr. Dieter Urban
January 1, 2008

ARTICLE TOOLS
EmailEmailPrintPrintReprintsReprintsshareShare



Figure 1.
Figure 1. Film structure seen in an AFM picture of a mono-modal dispersion. Tapping mode: dark areas = soft, bright = hard phases
Editor’s note: This paper was awarded the Pressure Sensitive Tape Council’s 2007 Carl A. Dahlquist Award for Best Technical Paper.

Acrylic polymers for pressure-sensitive adhesives (PSA) have been known to researchers for a long time. Polyacrylates with a specific monomer composition can be used as PSA without additional compounding or formulation. The application properties of polyacrylates adhesives are, therefore, mainly achieved through the polymer properties. More accurately, the film properties of the polymer determine the application properties of such adhesives.

Polyacrylates can be synthesized through solution- and emulsion polymerization, and can be applied as dispersion, a solution or as a reactive hot melt. Films that are formed from solution and reactive hot melts are mainly smooth and structure free, whereas polymer films formed from dispersions have well-defined structures (see Figure 1). The figure shows an AFM picture of a mono-modal dispersion after drying for 3 minutes at 90°C and then being cryo cut. The boundary areas of the former polymer particles are clearly seen, even though the film was completely dried. The question arises whether these structures that are found influence our adhesive properties and, if so, can we control these structures or application properties?


Enlarge this picture
Figure 2.
Figure 2. An illustration of the inverse proportionality that exists between peel and shear.
Important application properties of PSAs are peel and shear strength, which are known to be inversely proportional to each other (see Figure 2). Increasing shear resistance usually leads to a drop in peel force and vice versa. Usually, one aims to increase at least one property without loss of the other. Ultimately, one would like to increase both properties, as seen in Figure 2.

The aim of this research was to obtain specific polymer particle structures in waterborne acrylics that provide structured films with high performance application properties, increasing both shear and peel strength.


Structured Particles

Enlarge this picture
Figure 3.
Figure 3. Two-stage emulsion polymerization to create structured polymer particles.
Methods for creating structured particle morphologies in emulsion polymerization have been known for several years.1 Usually, a two-stage polymerization process is performed. In the first stage, an emulsion with a certain composition is fed into the reactor, followed by the second stage with another composition. Depending on the thermodynamic equilibrium as well as the kinetics of the polymerization, different particle morphologies can be obtained.  As shown in Figure 3, a swelling polymerization process can lead to heterogeneous structures of varying size. Here, small domains depending on the thermodynamic and kinetic factors are obtained; for example, Figure 3 shows a “raspberry” structure. During film formation, the structured polymer particles form structured films. The morphology of these films may or may not resemble the particle morphology, thus resulting in different application properties.


Enlarge this picture
Figure 4.
Figure 4. Tensile strength of three different polymers, each made of 75% BA and 25% MMA (white line shows  two-stage polymer, yellow line shows one-stage copolymer, and orange line is blend of 75%PBA and 25%PMMA).
To illustrate the effect of such micro-phase separated films, three tensile tests were performed on three different polymers, each having a composition of 75% PnBA and 25% PMMA (see Figure 4). The samples were 1.) a blend of the homopolymer dispersions; 2.) a statistical emulsion copolymerization of the monomers; and 3.) a two-stage emulsion polymerization (Stage 1: 75% BA, Stage 2: 25% MMA) resulting in phase-separated polymer particles. The results show that an increase in tensile strength occurs when a blend is made instead of a statistical copolymerization. This effect is enhanced when micro-phase separated domains are created during a two-stage polymerization within a polymer film instead of the macro-phase separated domains seen during blending.


Controlling the Morphology of Structured Particles

Enlarge this picture
Figure 5.
Figure 5. Cross-sections of dried dispersions with different chemical composition and morphology [TM-AFM phase images, 2µm × 2µm]. Different columns illustrate dispersions with different carboxylic acids, whereas the changes implied by swelling polymerization are shown in different rows. The insets are used to schematize the observed particle morphology.
As mentioned earlier, the morphology of dispersion particles can be controlled thermodynamically or kinetically.2 In a fundamental study, the effect of the acid type (acrylic acid, methacrylic acid and itaconic acid) on dispersion particles with different morphologies (no morphology, styrene microphases and methyl methacrylate microphases) was investigated. The different particle morphologies as seen through an atomic force microscope are seen in Figure 5. Figure 6 shows the results of shear and peel testing of the dispersions, formulated with 25% of tackifier resin.


Enlarge this picture
Figure 6.
Figure 6. Shear and peel (*) of dried dispersions with different chemical compositions and morphologies, as was shown in Figure 6.
Due to the low polymerization constant (kp) of styrene as well as the high hydrophobicity, the polystyrene domains are predominantly found inside the polymer particles. In the case of polymethyl methacrylate (PMMA), the particles are distributed between the surface and the inner part of the dispersion particles. Combining MMA and methacrylic acid (MAA) resulted in the highest shear and peel strengths. In the latter case, an optimal balance between phase-separated domains on the surface and inside of the polymer particles is formed.

These results further emphasize the importance of micro-phase separation in polymer films to enhance application properties.


Polymer Films with Structures Resembling Bi-Continuous Structures

Figure 7.
Figure 7.  2-D structure of a binary polymer solution after spinodal de-mixing showing bi-continuous phases.
The question that arises is whether it would be possible to create bi-continuous polymer films from structured polymer particles. While the analysis of bi-continuous structures in films is difficult, our aim was to find a phase-separated polymer film that resembled a 2D-structure of a binary polymer solution after spinodal de-mixing (see Figure 7).


Enlarge this picture
Figure 8.
Figure 8. Cross-sections of dried dispersion films (Dispersion A, Dispersion B, a mixture of A and B, as well as a two-stage polymer with the composition of A and B) measured by AFM [TM-AFM phase images, 2µm × 2µm].
For this purpose, the compositions of two test dispersions were used, namely a low-cohesive dispersion (A) and a high-cohesive dispersion (B). A two-stage polymerization, as shown before, was used to synthesize the structured particles. Films from the structured particles were compared to films from the original dispersions, as well as to a film of the blend from the original two dispersions. The AFM pictures of the films are seen in Figure 8.

In the AFM pictures of the original dispersions, the boundary structures mentioned before are clearly seen. This is also the case in the mixture, although the film is phase-separated. A totally different picture is seen for the film of the two-stage polymer. Here a microphase-separated film is seen with no structures between the polymer particles. In fact, one is not even able to distinguish the different particles, which were 200 nm large.


Enlarge this picture
Figure 9.
Figure 9. Comparison of the adhesive properties of a mixture of Dispersion A and Dispersion B and the stage polymer with the composition of A and B. 
The application properties of the films were tested, the results of which are shown in Figure 9. The stage-emulsion polymerization polymer film that resembles a bi-continuous film structure exhibits the best combination of properties. Both peel and cohesion properties of a tailor-made emulsion polymer are superior compared to a mixture of single-emulsion polymers having the same chemical composition. The important difference between mixtures of emulsion polymers and tailored emulsion polymers is the resulting film morphology. The advanced design of waterborne adhesive results in better properties than those that can be achieved by blending.


Summary

A tailored particle morphology achieved by a staged-emulsion polymerization process provides special polymer film morphologies. Either small-sized polymer domains or bi-continuous film structures provide premium adhesive properties, which cannot be obtained by a blending process. Advanced polymer design, well-fitting formulation know-how and the newest coating technology continuously result in new classes of high-performance adhesives. And we are happy to provide all of this to our customers in order to make them more successful.


Acknowledgements

Michael Kutschera, Ph.D., BASF-AG, Ludwigshafen, Germany

Nok-Young Choi, Ph.D., BASF-AG, Ludwigshafen, Germany


Dr. Cornelis Beyers
Cornelis Beyers is a representative of BASF-AG, Ludwigshafen, Germany.

Dr. Petra Schöcker
Petra Schöcker is a representative of BASF-AG, Ludwigshafen, Germany.

Dr. Dieter Urban
Dieter Urban is a representative of BASF-AG, Ludwigshafen, Germany.

Dr. Stefan Kirsch
Stefan Kirsch is a representative of BASF-AG, Ludwigshafen, Germany.

References
1. Durant, Y.; Sundberg, D.C. (1995), J. Appl. Polym. Sci., 58, pp. 1607-1618.
2. Kirsch, S.; Choi, N-Y.; Kutschera, M.; Frechen, T. (2006), J. Appl. Polym. Sci., 101, pp. 1444-1455.

|PrintEmail

Did you enjoy this article? Click here to subscribe to the magazine.