Adhesives Mag logo
search
cart
facebook twitter linkedin youtube
  • Sign In
  • Join Today
  • Sign Out
  • My Account
Adhesives Mag logo
  • NEWS
    • Latest Headlines
    • ASI News Now
    • Mergers/Acquisitions
    • Market Trends
    • TOP 20
  • NEW PRODUCTS
  • TOPICS
    • Finished Adhesives and Sealants
    • Pressure-Sensitive Adhesives (PSAs)
    • Coatings
    • Raw Materials and Chemicals
    • Materials Handling/Processing
    • Meter/Mix/Dispense
    • Curing
    • Testing/Quality Control
    • Packaging of Adhesives & Sealants
    • Converting/Packaging
    • Composites
    • Sustainability
  • COLUMNS
    • From the Editor
    • Strategic Solutions
    • Supply Chain Strategies
    • Tape Talk
  • EVENTS
    • ASI Academy
    • Events Calendar
  • MULTIMEDIA
    • Videos
    • Podcasts
    • Webinars
    • eBooks
  • DIRECTORIES
    • Buyers' Guide
    • Equipment Handbook
    • Global Adhesives & Sealants Directory
    • Raw Materials, Chemicals, Polymers and Additives Handbook
  • EXPLORE
    • Adhesives in Action
    • Blog
    • ASI Store
    • Industry Links
    • Market Research
    • Sponsor Insights
    • Classifieds
  • EMAGAZINE
    • EMAGAZINE
    • ARCHIVE ISSUES
    • ADVERTISE
    • CONTACT
  • JOIN!
Adhesives and Sealants TopicsInfo For...Testing/Quality ControlFormulatorsManufacturers

Rheology Solutions for Adhesives Testing

By John Walters
October 1, 2011
When testing adhesive materials, dual capability is vital to the range of necessary rheological tests.



Controlled stress rheometers with cone/plate or plate/plate geometry are ideally suited for a variety of adhesive measurements. They also have the capability to apply a defined shear rate to the adhesive material. These instruments can operate in either controlled stress mode for yield stress, creep and recovery tests, or at a controlled rate for viscosity testing.

The following performance capabilities are important in a versatile controlled stress instrument for running a wide range of rheological tests:
  • Controlled stress capability, with ramping up to several thousand Pascals
  • Defined shear rate capability, with ramping up to several thousand reciprocal seconds
  • Small sample volume on the order of 1-5 mL, depending on spindle geometry
  • Fast, easy cleanup
  • Wide temperature range, preferably from 0-200ºC
  • Fast temperature change, possible when using peltier technology; instruments can change from ambient temperature to 100°C (or vice versa) in five minutes or less
  • High torque range up to 50 mNm for measuring thick materials
  • Spindle geometries with cones and plates of various diameters that allow measurement of viscosities from ~100 cP (100 mPa·s) to >15,000,000 cP (15,000 Pa·s)
The following examples describe potential uses of controlled stress rheometers.

Figure 1. Viscosity vs. Shear Rate for Two Adhesives

Viscosity vs. Shear Rate for Two Adhesives

As shown in Figure 1, a simple speed ramp from 0 sec-1 to 100 sec-1 tests two variations of an adhesive. The adhesive indicated by the data shown in red performs well; the green, less so.

Tests with a conventional viscometer at one speed produced similar viscosity values. The test with the rheometer over the shear rate range in the figure clearly shows that the green material, while near the red at low shear rates, thins and seems to become unstable at shear rates over 20 sec-1. If the adhesive is applied at fairly high shear rates, the green formulation will not work.

Figure 2. Shear Stress Ramp (Red) and Viscosity Profile (Green)

Shear Stress Ramp and Viscosity Profile

Yield stress (i.e., the point at which flow begins) can be an important property. Many consumer adhesives are supplied in tubes that the consumer squeezes the adhesive out of. If too much force is required to initiate flow, the product may not be acceptable to consumers. Using a controlled stress instrument, a simple stress ramp provides a precise yield stress value.

In Figure 2, shear stress is ramped from 0 Pa to ~ 600 Pa over 60 seconds. Because the adhesive does not move until the yield stress is achieved, there is no shear rate (and hence viscosity) until yield takes place. The graph clearly shows that the yield stress value for this adhesive is ~ 50 Pa (see the curve in red), which is an acceptably low value.

In addition, this graph shows that the adhesive is pseudoplastic (i.e., exhibits decreasing viscosity with increasing shear rate), so the viscosity will decrease as the consumer squeezes the tube (see the curve in green). The consumer will not need to squeeze the tube with significant force, and the adhesive will be easily applied.

Figure 3. Viscosity vs. Shear Rate Up-Down Test to Assess Recovery

Viscosity vs. Shear Rate Up-Down Test

When the adhesive is supplied in a tube or container, force is required for application of the material. Viscosity recovery may be an issue. As force is applied and the shear rate increases, the viscosity will probably change (most commonly, it will decrease). After having been sheared, if the material does not recover to a fairly high viscosity, it may not “stay where it is put,” which can be a problem. A simple two-step flow curve, which only takes two minutes, assesses both the degree of shear thinning behavior and the recovery.

The test program has two steps. In the first step, shear rate is ramped from 0 sec-1 to 300 sec-1; in step two, it is ramped from 300 sec-1 to 0 sec-1. As is evident in Figure 3, viscosity in the first step drops dramatically from ~ 80 Pa·s (80,000 cP) at low shear rates to ~ 5 Pa·s (5,000 cP) at 300 sec-1. In the second step, some “interesting” behavior then begins at about 160 sec-1. Although the step-two viscosity values are less than the step-one values for any given shear rate, there is recovery and the final viscosity reading of ~ 52 Pa·s (52,000 cP) will be high enough for the adhesive to stay where it is applied.

Figure 4. Two-Point QC Test

Two-Point QC Test

While viscosity data taken over multiple rotational speeds provides more information about the fluid flow properties, a quick QC test can be accomplished with two data points: one at high shear rate and the other at a low shear rate. To further simplify the test procedure, this type of test can be done without PC control (though using a printer is recommended).

In Figure 4, viscosity readings are taken at 10 sec-1 and 500 sec-1. The printed output displays viscosity under the term “Eta” and the two values noted are 15.410 Pa·s and 1.279 Pa·s, respectively. This clearly indicates a significant degree of shear thinning behavior, which is desirable for good adhesive performance when in use. Note that all measured values are printed, as well as instrument and program information.

Figure 5. Math Model Analysis of Viscosity Data Using the Oswald Regression

Math Model Analysis of Viscosity Data Using the Ostwald Regression

When a controlled stress rheometer is under software control, the ability to apply a regression analysis to the test data offers a significant opportunity to analyze the data quickly and effectively. With good correlation, this allows the estimation of viscosity values at untested shear rates.

Figure 5 shows the Ostwald (power law) regression for a nearly Newtonian fluid having a viscosity of ~ 250 Pa·s (250,000 cP). It would take considerably more torque capability in an instrument to test the fluid at a shear rate of 1000 sec-1 (a 30-hp rheometer would be quite expensive). Because the correlation to the Ostwald model is good (99.628, in this case), we can use the model to estimate the viscosity at 500 sec-1 and 1,000 sec-1. The values were 246.725 Pa·s and 246.090 Pa·s, respectively, seen at the end of the results where stress and rate are also shown. The Ostwald n and k values are shown as constants 1 and 0; the n is 0.9962 while the k is 252.489 Pa·s.

Figure 6. Viscosity vs. Shear Rate for Highly Viscous Adhesive

Viscosity vs. Shear Rate for Highly Viscous Adhesive

Figure 6 shows the high viscosity capability of the controlled stress rheometer. The test was a simple stress ramp up to ~ 6,100 Pa using 25 mm flat plate geometry. Note that at low shear rates (below 1 sec-1), the viscosity was well over 1,000 Pa·s (1,000,000 cP). Testing fluids that are highly viscous at defined shear rates is nearly impossible with other moderately priced instruments.

Figure 7. Vane Spindle Rotation vs. Time Measures "Stiffness"

Vane Spindle Rotation vs. Time Measures "Stiffness"

This application uses the vane spindle with a controlled stress rheometer. Vane spindles are useful for low shear measurement of very high-viscosity, near-solid materials. In this case, a heavy flooring adhesive served as the sample.

The test includes two steps, using stress (or torque) as the control parameter. In step one, a constant stress or torque is applied. In step two, the stress/torque is removed. This provides a measurement of stiffness by plotting the movement of the vane (in radians) against time. Less stiff materials have more movement. By removing stress/torque in step two, it is possible to get an indication of the degree of elastic behavior; more elastic materials will pull the vane back toward the start point. In this example, the red, light green and green samples were acceptably stiff; the purple sample was not sufficiently rigid (see Figure 7).

Dual Capability

The examples presented here serve to provide a sense of a controlled stress rheometer’s capabilities. The important point to keep in mind is that this type of instrument operates in both controlled stress and controlled rate modes. When testing adhesive materials, this dual capability is vital to the range of necessary rheological tests. The shift to the use of controlled stress instrumentation is a logical step toward ensuring that R&D and QC labs operate at peak efficiency.

For additional information, contact Brookfield Engineering Laboratories, Inc. at 11 Commerce Blvd., Middleboro, MA 02346; phone (800) 628-8139; fax (508) 946-6262; email the author at j_walters@brookfieldengineering.com; or visit www.brookfieldengineering.com.

Links

  • Brookfield Engineering Laboratories
KEYWORDS: rheology shear testing viscosity testing

Share This Story

Looking for a reprint of this article?
From high-res PDFs to custom plaques, order your copy today!

John Walters is a senior engineering and R/S product manager for Brookfield Engineering Laboratories, Inc.

Recommended Content

JOIN TODAY
to unlock your recommendations.

Already have an account? Sign In

  • 2026 ASI Top 20: Leading Global Adhesives and Sealants Manufacturers

    2026 ASI Top 20: Leading Global Adhesives and Sealants Manufacturers

    Every year, we study the leading worldwide manufacturers...
    Pressure-Sensitive Adhesives (PSAs)
    By: Karen Parker
  • PSA Market

    Trends and Opportunities in Pressure-Sensitive Adhesives: Sustainability, Innovation, and Market Growth

    The pressure-sensitive adhesives market is growing...
    Pressure-Sensitive Adhesives (PSAs)
    By: Chirag Tripathi and Parag Shah
  • science test tubes

    2026 Adhesives and Sealants Raw Materials Roundup

    After more than two years of contraction, the...
    Sustainability
    By: Karen Parker
Manage My Account
  • Join Adhesives & Sealants Industry
  • Manage My Preferences
  • Customer Service

More Videos

Sponsored Content

Sponsored Content is a special paid section where industry companies provide high quality, objective, non-commercial content around topics of interest to the Adhesives and Sealants Industry audience. All Sponsored Content is supplied by the advertising company and any opinions expressed in this article are those of the author and not necessarily reflect the views of Adhesives and Sealants Industry or its parent company, BNP Media. Interested in participating in our Sponsored Content section? Contact your local rep!

close
  • Industrial robot performing plasma surface treatment on an automotive component
    Sponsored byPlasmatreat North America

    Engineering the Molecular Interface: Atmospheric Plasma Cleaning and Activation for Reliable Bonding

  • Assembly automation for medical device manufacturing
    Sponsored byNordson EFD

    Three Proven Principles Powering Quality Assembly

Popular Stories

news on internet screen

Ancora Calls for Potential Sale of H.B. Fuller

Photo of a person holding a tablet, reading a new story

H.B. Fuller Rejects Ancora’s Second Offer for Building Adhesive Solutions Business

Image of scrabble pieces with pictures of people

Sika Acquires UAE Waterproofing Firm Duproof

ASI 2026 Top 20 Adhesives & Sealants List

Events

January 1, 2030

Webinar Sponsorship Information

For webinar sponsorship information, visit www.bnpevents.com/webinars or email webinars@bnpmedia.com.

View All Submit An Event

Products

Adhesives Technology Handbook   3rd Edition

Adhesives Technology Handbook 3rd Edition

See More Products

Related Articles

  • aerial shot of footpath through dense forest

    Challenges in Developing Sustainable Packaging Solutions for Adhesives

    See More
  • Photo-3-Jet-valves-remove-the-barrier-between-speed-and-accuracy,--making-them-the-most-precise-dispensing-equipment-in-the-field

    Common Dispensing Challenges and Solutions for Adhesives and Other Materials

    See More
  • Top-image.jpg

    Sustainable Material Pretreatment and Activation Solutions for Adhesives and Sealants

    See More

Related Directories

  • Capital Adhesives Inc.

    Capital Adhesives is an American-owned manufacturer of industrial adhesives and coatings, including hot melt adhesives, water-based adhesives, and custom formulations. Since 1987, we have served packaging, paper converting, graphic arts, and product assembly manufacturers with reliable products, responsive technical support, consistent quality, and solutions designed to keep production moving efficiently.
×

Keep the info flowing with our newsletters!

Get the latest industry updates tailored your way.

JOIN TODAY!
  • RESOURCES
    • Advertise
    • Contact Us
    • Directories
    • Manufacturing Division
    • Store
  • JOIN TODAY
    • Create Account
    • eMagazine
    • Newsletters
    • Customer Service
    • Manage Preferences
  • SERVICES
    • Marketing Services
    • Reprints
    • Market Research
    • List Rental
    • Survey & Sample
  • STAY CONNECTED
    • LinkedIn
    • Facebook
    • Youtube
    • X (Twitter)
  • PRIVACY
    • PRIVACY POLICY
    • TERMS & CONDITIONS
    • DO NOT SELL MY PERSONAL INFORMATION
    • PRIVACY REQUEST
    • ACCESSIBILITY

Copyright ©2026. All Rights Reserved BNP Media, Inc. and BNP Media II, LLC.

Design, CMS, Hosting & Web Development :: ePublishing